Creep behavior of an advanced magnesium alloy AX41 (4 wt.% Al, 1 wt.% Ca, Mg balanced) was investigated in temperature interval from 343 to 673 K and stresses from 2 to 200 MPa. Compressive creep experiments with stepwise loading were used in order to obtain stress dependence of the creep rate in interval from 10~9 to 10~3 iT 1 fo r a given temperature. All stress dependences can be well described by the Garofalo sinh relationship with natural exponent n = 5. An analysis ofthe parameters of this relationship has shown that lattice diffusion controls creep at all experimental conditions. While climb-controlled creep mechanism is decisive at lower stresses
and higher temperatures, glide-controlled mechanisms act at higher stresses and lower temperatures. A typical power-law breakdown is observed at intermediate stresses and temperatures.
Выполнены исследования ползучести оптимизированного
магниевого сплава AX41 (4
вес.% Al, 1 вес.% Ca, Mg - баланс) в температурном
диапазоне 343...673 K и уровнях
напряжений 2...200 МПа. Были проведены
испытания на ползучесть при ступенчатом
нагружении сжимающей нагрузкой с целью
определения зависимости скорости ползучести
от напряжения в диапазоне 10-9...10-3
с-1 для данной температуры. Все вышеуказанные
зависимости хорошо описывались
уравнением Барафоло (типа sinh) с
показателем степени n = 5. Анализ параметров
этого уравнения показал, что ползучесть
во всех проведенных экспериментах
определяется диффузией решетки. При низких
уровнях напряжений и высоких температурах
определяющим является механизм
восхождения, а при высоких уровнях напряжений
и более низких температурах - механизм
скольжения. В промежуточном диапазоне
напряжений и температур наблюдается
характерное отклонение экспериментальных
точек от степенной зависимости.